Group 1.10 Pressure-Temperature Ratings
2.25Cr-1Mo alloy steel. The standard refinery heater and reformer material, chosen over Group 1.9 for its better high-temperature creep strength and hydrogen service resistance.
- Standard
- ASME B16.5
- Group
- Group 1.10
- Materials
- A182 F22 Cl. 3, A217 WC9, A387 Gr. 22 Cl. 2
- Class 150 at 100 °F
- 290 psig (20.0 bar)
- Class 150 at 600 °F
- 140 psig (9.7 bar)
| Class | 100 °F | 200 °F | 300 °F | 400 °F | 500 °F | 600 °F | 650 °F | 700 °F | 750 °F | 800 °F | 850 °F | 900 °F | 950 °F | 1000 °F |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Class 150 | 290 | 260 | 230 | 200 | 170 | 140 | 125 | 110 | 95 | 80 | 65 | 50 | 35 | 20 |
| Class 300 | 750 | 750 | 730 | 705 | 665 | 605 | 590 | 570 | 530 | 510 | 485 | 450 | 385 | 265 |
| Class 400 | 1000 | 1000 | 970 | 940 | 885 | 805 | 785 | 755 | 710 | 675 | 650 | 600 | 515 | 355 |
| Class 600 | 1500 | 1500 | 1455 | 1410 | 1330 | 1210 | 1175 | 1135 | 1065 | 1015 | 975 | 900 | 775 | 535 |
| Class 900 | 2250 | 2250 | 2185 | 2115 | 1995 | 1815 | 1765 | 1705 | 1595 | 1525 | 1460 | 1350 | 1160 | 800 |
| Class 1500 | 3750 | 3750 | 3640 | 3530 | 3325 | 3025 | 2940 | 2840 | 2660 | 2540 | 2435 | 2245 | 1930 | 1335 |
| Class 2500 | 6250 | 6250 | 6070 | 5880 | 5540 | 5040 | 4905 | 4730 | 4430 | 4230 | 4060 | 3745 | 3220 | 2230 |
Interpolation between listed temperatures is permitted; extrapolation is not.
How far this table has been checked. The Class 400 row rests on a single secondary source. The other classes agree in two independent sources. None of the values on this site has been checked against the standard itself; see how the figures are checked.
What Group 1.10 is used for
This is the 2¼Cr-1Mo chrome-moly group. It is used for high-temperature steam and for hot hydrogen service in refineries, where the alloy content resists both creep and hydrogen attack.
Reading the ratings
A Class 300 flange in Group 1.10 is rated 750 psig at 100 °F, 605 psig at 600 °F and 265 psig at 1000 °F, which is 35% of its cold rating. Every other class in the group follows the same curve, scaled by the class. It is at or above Group 1.1 carbon steel at every temperature in the table: at 1000 °F carbon steel is down to 85 psig in the same class.
Each figure is the highest gauge pressure the flange may see at that metal temperature. To use the table, fix the material group and the design temperature first, read down to find the lowest class whose rating is at or above the design pressure, and interpolate between columns if the temperature falls between them. The rating of the flange is often what limits a line, since the pipe wall is usually good for more.
Guides and comparisons for this page
Common questions
Which materials are in ASME B16.5 Group 1.10?
A182 F22 Cl. 3, A217 WC9, A387 Gr. 22 Cl. 2.
What is a Class 300 Group 1.10 flange rated at 600 °F?
605 psig (41.7 bar). At 100 °F the same flange is rated 750 psig (51.7 bar).